This isn't so much a new feature as it is a cleaning up of the output for EDS and WDS integrated samples.
If you have both analyzed EDS and WDS elements in your run, the output for say the Data button in the Analyze! window will look like this:
Un 7 Mg2SiO4
TakeOff = 40.0 KiloVolt = 15.0 Beam Current = 20.0 Beam Size = 10
(Magnification (analytical) = 20000), Beam Mode = Analog Spot
(Magnification (default) = 2524, Magnification (imaging) = 736)
Image Shift (X,Y): .00, .00
Number of Data Lines: 3 Number of 'Good' Data Lines: 3
First/Last Date-Time: 02/19/2013 04:18:02 PM to 02/19/2013 04:23:47 PM
Stage (or Beam Deflection) Coordinate Positions:
X Y Z X Y Z
18G 12260.00 -4962.000 11.00000 19G 12184.00 -4958.000 11.00000
20G 12145.00 -4958.000 11.00000
Sample Coordinates Referenced to Fiducial Set 2 C:\UserData\StandardPOSData\alkali-glass_pos4.pos
1 13206.0 4623.00 -26.000
2 19447.0 -4695.0 -61.000
3 6142.00 -4967.0 17.0000
Sample is a Time Dependent Intensity (TDI) Self-Calibration Acquisition Type Sample
On and Off Peak Positions:
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
ONPEAK 46273.0 42618.0 38444.0 23831.0 68281.0 .000000 .000000
OFFSET 89.8477 158.785 -44.414 208.352 10.3984 .000000 .000000
HIPEAK 47601.0 43683.0 39895.5 25367.9 68772.5 .000000 .000000
LOPEAK 44687.3 41392.0 37178.4 22782.5 67593.0 .000000 .000000
HI-OFF 1328.00 1065.02 1451.48 1536.89 491.500 .000000 .000000
LO-OFF -1585.7 -1226.0 -1265.6 -1048.5 -687.96 .000000 .000000
PHA Parameters:
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
DEAD: 3.00 3.31 3.25 3.31 2.97 .00 .00
BASE: .56 .56 .56 .50 .56 .00 .00
WINDOW 4.00 4.00 4.00 4.00 4.00 .00 .00
MODE: -1 -1 -1 -1 -1 0 0
GAIN: 2321. 1181. 567. 780. 700. . .
BIAS: 1300. 1850. 1330. 1850. 1840. . .
Last (Current) On and Off Peak Count Times:
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
BGD: OFF OFF OFF OFF OFF EDS EDS
BGDS: LIN LIN LIN LIN LIN EDS EDS
SPEC: 1 3 2 3 5 0 0
CRYST: TAP LPET LPET LPET LIF EDS EDS
ORDER: 1 1 1 2 1 1 1
ONTIM: 20.00 10.00 20.00 10.00 12.00 80.00 80.00
HITIM: 5.00 5.00 5.00 5.00 3.00 40.00 40.00
LOTIM: 5.00 5.00 5.00 5.00 3.00 40.00 40.00
UNFAC: 3 2 3 2 4 1 1
ONTIME 60.00 20.00 60.00 20.00 48.00 80.00 80.00
HITIME 15.00 10.00 15.00 10.00 12.00 40.00 40.00
LOTIME 15.00 10.00 15.00 10.00 12.00 40.00 40.00
Miscellaneous Sample Acquisition/Calculation Parameters:
KILO: 15.00 15.00 15.00 15.00 15.00 15.00 15.00
ENERGY 1.041 3.313 3.691 5.895 4.509 1.254 1.740
EDGE: 1.073 3.608 4.039 6.539 4.967 1.305 1.839
Eo/Ec: 13.98 4.16 3.71 2.29 3.02 11.49 8.16
STDS: 336 374 358 25 22 12 14
TDI#: -1 -1 -1 0 -1 0 0
EDS Spectrum Parameters (for datarow=1):
Time Constant= 0, Clock Time= 50.0
Elapsed Time= 126.2, Dead Time(%)= 37.
Live Time= 80.0, Channels= 2048
Ev Per Chan= 10, Max Counts= 211125
On-Peak (off-peak corrected) or MAN On-Peak X-ray Counts (cps/1nA) (and Faraday Current):
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka BEAM
BGD: OFF OFF OFF OFF OFF EDS EDS
SPEC: 1 3 2 3 5 0 0
CRYST: TAP LPET LPET LPET LIF EDS EDS
ORDER: 1 1 1 2 1 1 1
18G -.03 .13 .14 -.38 -.01 998.44 489.54 20.019
19G -.03 .00 .18 .02 .00 1000.83 489.85 20.014
20G -.02 .04 .15 .16 .00 996.85 488.16 20.014
AVER: -.03 .06 .16 -.06 .00 998.71 489.18 20.016
SDEV: .01 .07 .02 .28 .01 2.01 .90 .003
1SIG: .02 .05 .03 .11 .01 .79 .55
SIGR: .38 1.43 .82 2.61 .77 2.54 1.63
SERR: .00 .04 .01 .16 .00 1.16 .52
%RSD: -23.90 115.87 15.58 -442.29 -132.10 .20 .18
Off-Peak (calculated) X-ray Counts (cps/1nA):
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
TYPE: LINEAR LINEAR LINEAR LINEAR LINEAR AVERAGE AVERAGE
18G .36 .85 .90 4.84 .06 .00 .00
19G .35 .84 .92 4.72 .06 .00 .00
20G .35 .80 .89 4.59 .05 .00 .00
AVER: .36 .83 .90 4.72 .06 .00 .00
SDEV: .01 .03 .02 .12 .01 .00 .00
Raw Hi-Peak X-ray Counts (cps/1nA):
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
18G .36 .77 .82 4.39 .07 .00 .00
19G .28 .81 .84 4.21 .08 .00 .00
20G .31 .81 .81 3.97 .05 .00 .00
AVER: .32 .80 .82 4.19 .07 .00 .00
SDEV: .04 .02 .02 .21 .02 .00 .00
1SIG: .03 .06 .05 .14 .02 .00 .00
SIGR: 1.24 .35 .29 1.45 1.05 .00 .00
Raw Lo-Peak X-ray Counts (cps/1nA):
ELEM: na ka k ka ca ka mn ka ti ka mg ka si ka
18G .37 .94 .97 5.15 .04 .00 .00
19G .44 .88 1.00 5.06 .04 .00 .00
20G .39 .80 .96 5.02 .05 .00 .00
AVER: .40 .87 .98 5.08 .04 .00 .00
SDEV: .04 .07 .02 .07 .01 .00 .00
1SIG: .04 .07 .06 .16 .01 .00 .00
SIGR: .97 1.06 .36 .41 .48 .00 .00
Note that the peak positions and PHA parameters for the Mg Ka and Si Ka (as EDS elements) are zeros because, they aren't "useful". I'll probably make them dashes at some point (along with the off-peak intensity output)... which reminds me: I wish Thermo (and Bruker?) software sent back the EDS background intensities so I can calculate statistics for the EDS elements...
But if you decide to run PFE using *only* EDS elements (that is, no WDS elements), then it makes no sense to output the peak positions and PHA parameters at all, so this is the output you will now see for EDS only elements in PFE:
St 912 Set 1 MgO (elemental) (#12)
TakeOff = 40.0 KiloVolt = 15.0 Beam Current = 30.0 Beam Size = 0
(Magnification (analytical) = 40000), Beam Mode = Analog Spot
(Magnification (default) = 400, Magnification (imaging) = 800)
Image Shift (X,Y): .00, .00
1. UCB # M3567, 99.8%, EPMA (UCB): Ca ~ 0.2%
2. C. M. Taylor, 99.98%, EPMA (UCB) Ca ~ 0.02%
Number of Data Lines: 4 Number of 'Good' Data Lines: 4
First/Last Date-Time: 11/17/2014 06:17:30 PM to 11/17/2014 06:24:24 PM
Stage (or Beam Deflection) Coordinate Positions:
X Y Z X Y Z
26G -13078.00 26512.00 19.00000 27G -13074.00 26512.00 19.00000
28G -13070.00 26512.00 19.00000 29G -13066.00 26512.00 19.00000
Sample Coordinates Referenced to Fiducial Set 1 C:\UserData\StandardPOSData\STBLK1_pos1.pos
Last (Current) On and Off Peak Count Times:
ELEM: ni ka cr ka co ka fe ka cu ka al ka o ka
BGD: EDS EDS EDS EDS EDS EDS EDS
BGDS: EDS EDS EDS EDS EDS EDS EDS
SPEC: 0 0 0 0 0 0 0
CRYST: EDS EDS EDS EDS EDS EDS EDS
ORDER: 1 1 1 1 1 1 1
ONTIM: 59.90 59.90 59.90 59.90 59.90 59.90 59.90
HITIM: 29.95 29.95 29.95 29.95 29.95 29.95 29.95
LOTIM: 29.95 29.95 29.95 29.95 29.95 29.95 29.95
Miscellaneous Sample Acquisition/Calculation Parameters:
KILO: 15.00 15.00 15.00 15.00 15.00 15.00 15.00
ENERGY 7.473 5.412 6.926 6.400 8.041 1.487 .525
EDGE: 8.333 5.990 7.709 7.112 8.979 1.560 .532
Eo/Ec: 1.80 2.50 1.95 2.11 1.67 9.62 28.21
STDS: 528 524 527 526 529 513 912
EDS Spectrum Parameters (for datarow=1):
Time Constant= 0, Clock Time= 60.0
Elapsed Time= 125.7, Dead Time(%)= 52.
Live Time= 60.0, Channels= 2048
Ev Per Chan= 10, Max Counts= 389132
ELEM: ni ka cr ka co ka fe ka cu ka al ka o ka BEAM
BGD: EDS EDS EDS EDS EDS EDS EDS
26G .00 .00 .00 .09 .17 .00 368.54 29.916
27G .00 .00 .04 .18 .00 .00 368.86 29.911
28G .00 .00 .00 .27 .11 .00 372.59 29.908
29G .21 .00 .18 .00 .00 .00 369.28 29.902
AVER: .05 .00 .05 .14 .07 .00 369.82 29.909
SDEV: .11 .00 .09 .12 .09 .00 1.87 .006
1SIG: .01 .00 .01 .01 .01 .00 .45
SIGR: 19.51 .00 15.54 13.43 13.67 .00 4.13
SERR: .05 .00 .04 .06 .04 .00 .94
%RSD: 200.00 .00 158.28 86.27 121.83 .00 .51
A little more compact I think you all will agree!